New Publication
Publication · CEAS Space Journal · 2026

Integrated Electrical Connections in Deployable Composite Tube Flexures

Alberto Progida & Matthew J. Santer — Department of Aeronautics, Imperial College London

10.1007/s12567-026-00698-z
Material Samples

Overview

Spacecraft deployable booms and hinges rely on tube flexures — pairs of curved carbon-fibre tape springs that self-latch into a rigid deployed state and can be stowed compactly for launch. This paper introduces a method to make these structural hinges carry electrical signals and power at the same time, eliminating dedicated wire harnesses and reducing system mass.

The approach embeds a multi-layer conductive film at the midplane of the laminate: silver nanoparticle tracks are inkjet-printed onto a 25 µm Kapton substrate, then encapsulated in a thermoplastic polyolefin film to prevent short-circuits with the surrounding carbon fibres. The complete stackup — [+45/−45 / Kapton+Ag / PO / −45/+45] — is co-cured on a cylindrical mandrel under vacuum at 150 °C, producing a 127 µm-thick flexure with integral electrical traces.

Complete layup stackup illustration
Fig. 2 — The complete [+45/−45/Kapton+Silver Ink/PO/−45/+45] laminate stackup, with the conductive interleave embedded at the midplane. The staggered ply-drop geometry at each end exposes the track terminals while preventing short-circuits with the outer CFRP plies.

Assembly & Testing

Four tube flexures were manufactured — each comprising two tape springs bonded to 3D-printed couplers — and subjected to seven fold-unfold cycles on a custom bending rig. Moment and rotation were measured simultaneously with track resistance and RS-232 signal integrity, giving a complete picture of how the electrical and mechanical performances evolve together under repeated high-strain loading.

Render of assembled tube flexure
Fig. 7 — Render of a fully assembled tube flexure with four conductive tracks (two per spring). The 3D-printed couplers house PCBs for simple electrical connection, while clamp rings fix the tape springs at each end.

Test Setup

Each flexure was mounted between two thin-walled shafts instrumented with full-bridge strain gauge rosettes (±45° to the shaft axis), one fixed and one free to translate along a linear rail to maintain pure bending throughout the fold. End rotations were applied via worm-gear knobs and measured by analogue potentiometers at ±5.4 µ° resolution. Track resistance was logged continuously alongside moment and rotation using a Keysight 34410A multimeter, and RS-232 signal integrity was checked at the start and end of each fold.

Top-down photograph of the experimental test setup
Fig. 10 — Top-down photograph of the bending test rig with a flexure installed. One shaft is fixed while the other translates along a linear rail, ensuring pure bending. Worm-gear knobs drive the end rotations; potentiometers measure angle and strain gauges measure the applied moment.

Mechanical Results

The flexures behaved as expected structurally: a sharp peak moment followed by snap-through and a stable constant moment region. Repeated folding produced a statistically significant 32% reduction in peak locking moment between the first and subsequent folds — a "breaking-in" behaviour consistent with progressive compressive matrix damage — while snap angle and constant moment remained unchanged. Abaqus/Explicit quasi-static simulations with a 0.5° mounting misalignment matched first-fold peak moments to within 4%.

Moment-rotation dataset for Flexure 1
Fig. 12 — Moment-rotation dataset across seven successive folds for Flexure 1, overlaid with quasi-static FEA predictions for 0.0° and 0.5° mounting misalignments. The progressive reduction in peak moment is clearly visible; snap angle and constant moment are stable across folds.

Electrical & Thermal Results

No track failures were recorded across all 28 fold cycles. Every flexure successfully transmitted RS-232 data at 115,200 baud — the maximum standard rate — in both stowed and deployed configurations, and four flexures daisy-chained in series maintained full-rate communication. Power transmission was demonstrated at 2.5 W, with no measurable change in electrical resistance or signal quality over the test campaign. Resistive heating to ~50 °C was also achieved, but induced delamination-buckling failure at the silver-track/polyolefin interface during stowage — identifying bond strength as the critical barrier to shape-memory applications.

Infrared thermal imagery of power transmission
Fig. 16 — Infrared imagery of Flexure 2 transferring 101 mA at steady state. Spring 2B (higher resistance, 318 mW dissipated) shows a 4.0 °C rise above ambient versus 3.4 °C for Spring 2A.
SEM images of thermal failure
Fig. 21 — Scanning electron micrographs of the thermally induced delamination failure. The silver track is cracked and peeled from the Kapton substrate; lack of PO residue on the track surface indicates poor adhesion at the Ag–PO interface.

Key Findings

  • →RS-232 digital communication at 115,200 baud sustained in both deployed and fully stowed states, with up to four flexures daisy-chained in series.
  • →2.5 W power delivery demonstrated with no measurable degradation in resistance or signal quality over seven fold-unfold cycles.
  • →Resistive heating to ~50 °C is achievable in the deployed state, but causes delamination-buckling failure during stowage — bond strength improvement (plasma treatment, laser micro-texturing) is identified as the key next step.
  • →A 37% reduction in peak stiffness between folds is consistent with compressive matrix damage observed in non-interleaved flexures in prior studies, not attributable to the conductive interleave alone.